I tried adding solder to a reed tip today, but the solder would not stick to the reed. On the occasion when I managed to get some to stay on the reed tongue, it just popped right off after it hardened. Help? I have a temperature controlled iron and got it good and hot, I roughed up the surface of the reed tongue at the tip, and I’m using 50/50 solder with lead. Still no luck.
-
I've never had problems with 50/50 solder with flux (for electronics). Is that what you're using ?
-
It is essential that you clean the reed scrupulously, then I use some flux and prefluxed solder.
-
You need to file the reed where the solder will go. Fresh steel surface. Steel is harder to solder than brass or copper.
-
I roughed up the reed surface where it was to accept solder but that didn’t help. I’m not sure if the 50/50 solder I have has flux in it or not. Hardware stores aren’t open on Sundays here, but my neighbour says he has lead-free solder as well as flux, so I may try that.
-
I roughed up the reed surface where it was to accept solder but that didn’t help. I’m not sure if the 50/50 solder I have has flux in it or not. Hardware stores aren’t open on Sundays here, but my neighbour says he has lead-free solder as well as flux, so I may try that.
You need to do more than rough the surface up it needs to be clear of all contaminates
-
I roughed up the reed surface where it was to accept solder but that didn’t help. I’m not sure if the 50/50 solder I have has flux in it or not. Hardware stores aren’t open on Sundays here, but my neighbour says he has lead-free solder as well as flux, so I may try that.
You need to do more than rough the surface up it needs to be clear of all contaminates
Flux is a cleaner but I guess more cleaning cannot hurt.
I agree more of a grind on the surface as Theo and you suggest, flux is supposed to remove impurities and surface oxidizing, grinding / filing removes the oxidation quickly.
-
The reed itself needs to be hot enough to melt the solder. Slip a shim or pinger under the reed tip. Put the soldering iron tip on the reed for 10 or 20 seconds before introducing the (fluxed core) solder to preheat it. Push the solder right between where the iron and the reed are touching.
-
It was the flux (or lack thereof). Once I applied flux to the appropriate spot on the reed tongue, the solder stuck without any issue. In fact, I did away with the soldering iron entirely and simply placed a small piece of solder on the reed and melted it in place with a lighter. The entire process only took a few seconds and -presto- it was ready for filing. Thanks, all!
-
You probably know this, but keep a file cleaning wire brush to hand when filing lead. It clogs up files badly and quickly.
Dave.
-
Even better keep an old file for all filing of solder. It can be a coarser one than you would use on reed steel. It will still need to be cleaned after some use.
-
Yes, I have a coarse, cheap file on hand for filing weighted reed tips. I don’t use any of my good files for that.
-
You may have not gotten the reed itself hot enough, it needs to reach the melting temp of the solder to get a good bond.
Electrical solder typically has a lower melting point than say plumbing or tin smithing solder.